Scroll to turn the page
Materials Science · Structure
no crystal is perfect, and atoms move
The perfect crystals of Chapter 1 do not exist. Every real crystal has missing atoms, extra atoms, foreign atoms and misplaced planes, and those flaws decide much of how it behaves.
The figure shows two of them at work. On the left, a lattice site is empty: a vacancy. Again and again a neighbor (red) jumps into it, and the vacancy wanders the other way. On the right, a small atom (blue) sits in the gaps between larger ones and hops from gap to gap.
Both are diffusion: atoms moving through a solid. It is how steel is case-hardened, how dopants get into silicon, and why hot metals slowly change.
This chapter catalogs the imperfections, point, line and boundary, then measures diffusion: Fick’s laws, and the steep way diffusion speeds up with temperature.
how many sites are empty
A vacancy is a lattice site with no atom. Vacancies are not mistakes of manufacture: every crystal above absolute zero must have some, because the disorder they add lowers its free energy. Their equilibrium number rises steeply with temperature:
N is the number of atomic sites, Qv the energy to form one vacancy, k = 8.62 × 10−5 eV/(atom·K) is Boltzmann’s constant, and T in kelvins.
Example: copper at 1000 °C. Qv = 0.9 eV/atom; at this temperature ρ = 8.4 g/cm3, A = 63.5 g/mol. The number of sites per cubic meter:
About 2.7 × 10−4 of sites are empty, roughly one in 3600. At room temperature the equilibrium fraction is near 6 × 10−16. An atom can also be squeezed into a gap between sites: a self-interstitial, far rarer in metals because it distorts the lattice so much.
solid solutions, and how composition is counted
Pure metals are rare in use; most are alloys, with other elements dissolved on purpose. When the added atoms fit into the host’s crystal without forming a new structure, the result is a solid solution.
In a substitutional solid solution, solute atoms (red, left) take the place of host atoms. The Hume-Rothery rules say when that works over a wide range: atomic radii within about ±15%, the same crystal structure, similar electronegativities, and similar valences.
| host, solute | radius difference | structures | electroneg. | result |
|---|---|---|---|---|
| copper, nickel | −3% | FCC, FCC | 1.9, 1.9 | complete solubility |
| copper, zinc | 4% | FCC, HCP | 1.9, 1.6 | up to about 35 wt% Zn (brass) |
| iron (α), carbon | −43% | BCC, — | 1.8, 2.6 | interstitial, at most 0.022 wt% C |
In an interstitial solid solution, small atoms (red, right) sit in the gaps between host atoms. Carbon in iron is the key case: it strains the lattice, so little dissolves, and that little is what makes steel.
Composition is given in weight percent or atom percent. To convert from weight to atom percent,
For 5 wt% copper in aluminum: at% Cu: fewer atoms than the weight suggests, because copper atoms are heavier.
line defects, and how metals bend
A dislocation is a line defect: a row of atoms around which the lattice is out of register. In an edge dislocation, an extra half-plane of atoms (red) is wedged into the crystal, ending at the dislocation line, marked ⊥.
Push the top of the crystal one way and the bottom the other (blue). The dislocation does not need the whole top half to slide at once. Instead the bonds next to the extra half-plane switch partners one row at a time, and the dislocation glides along the slip plane. When it leaves the crystal, the top has moved by one atomic spacing.
That spacing is the Burgers vector b: the size and direction of the lattice distortion. In an edge dislocation b is perpendicular to the line; in a screw dislocation it is parallel, and the planes spiral around the line like a ramp. Most real dislocations are mixed. In FCC copper, b is half a face diagonal: a√2/2 = 0.2556 nm.
Moving a row at a time takes a small fraction of the force needed to slide whole planes, which is why real metals yield at stresses hundreds to thousands of times lower than a perfect crystal would need. Plastic deformation is dislocation motion (Chapter 4).
interfacial defects, and how they are seen
Planes of imperfection come in several kinds: the free surface, where atoms lack neighbors on one side; grain boundaries, where two grains of different orientation meet; and twin boundaries, where the lattice on one side mirrors the other.
Atoms at a grain boundary are less tightly bonded, so a boundary has an energy and is more reactive than the grain inside. Polish a metal and etch it with acid and the boundaries are attacked first: under a microscope they show as dark lines (the figure), each enclosed shape a grain.
Grain size is reported as an ASTM grain-size number G: at 100× magnification there are n grains per square inch of image, where
A larger G means more, smaller grains. For G = 6, n = 32 grains/in2 at 100×. At another magnification M, scale by (100/M)2: at 85×, 44.3 grains/in2.
how an atom gets from one site to the next
An atom vibrates about its site billions of times a second. Now and then it gains enough energy to break its bonds and jump. Two mechanisms carry most diffusion in metals.
Vacancy diffusion (left): an atom swaps places with a neighboring vacancy. Atoms and vacancies flow in opposite directions. It is how host atoms move (self-diffusion) and how substitutional solutes move, so its rate depends on how many vacancies there are, which climbs with temperature (2.1).
Interstitial diffusion (right): a small atom (blue) such as carbon, hydrogen or nitrogen hops from one interstitial gap to the next. There are always empty gaps to hop into, and small atoms squeeze through more easily, so interstitial diffusion is usually much faster than vacancy diffusion.
Both need an activation energy: the energy to squeeze past the neighbors on the way. That one fact is why diffusion depends so steeply on temperature (2.8).
Fick’s first law
Atoms jump in every direction, but where there are more of them on one side, more jump away from that side than toward it. The net flow runs down the concentration gradient.
The diffusion flux J is the mass (or number of atoms) crossing a unit area per unit time. When the profile does not change with time, steady state, Fick’s first law holds:
D is the diffusion coefficient (m2/s). The minus sign: atoms flow toward lower concentration.
Example. Carbon diffuses through a steel plate at 700 °C, where D = 3 × 10−11 m2/s. At 5 and 10 mm below the carbon-rich surface, the concentrations are 1.2 and 0.8 kg/m3:
Hydrogen purification works this way: hydrogen alone diffuses quickly through a thin palladium sheet, so gas on the far side is pure.
Fick’s second law, and case hardening
Most diffusion in practice is not steady: the profile changes with time. Then Fick’s second law governs it,
For a thick solid starting at C0, its surface held at Cs, the solution uses the error function, erf:
Carburizing hardens a steel surface by soaking it in a carbon-rich gas. Example. A 0.25 wt% C steel at 950 °C, surface held at 1.2 wt% C. How long until 0.8 wt% C at 0.5 mm? With carbon in FCC iron at 950 °C, D = 1.10 × 10−11 m2/s (from 2.8):
The figure runs the clock: the red profile sinks in, and passes 0.8 wt% at 0.5 mm (blue) at 10.3 h. Depth grows as √(Dt): twice the depth takes four times as long.
D = D₀ exp(−Q_d/RT)
Every jump needs an activation energy, so the diffusion coefficient climbs exponentially with temperature:
Plot log D against 1/T and each pair gives a straight line whose slope is −Qd/2.3R: steeper lines, larger activation energies.
| species | host | D0 (m2/s) | Qd (kJ/mol) | D at 900 °C |
|---|---|---|---|---|
| C | α-Fe (BCC) | 1.1 × 10−6 | 87.4 | 1.4 × 10−10 |
| C | γ-Fe (FCC) | 2.3 × 10−5 | 148.0 | 5.9 × 10−12 |
| Fe | α-Fe (BCC) | 2.8 × 10−4 | 251.0 | 1.9 × 10−15 |
| Cu | Cu | 7.8 × 10−5 | 211.0 | 3.1 × 10−14 |
Carbon, interstitial, diffuses many orders of magnitude faster than iron does in its own lattice. And carbon moves faster through BCC iron than FCC: the BCC lattice is less tightly packed. (At 900 °C iron is FCC; the BCC rows at that temperature are extrapolations of their lines.)
Example. Carbon in FCC iron at 950 °C: